Figure 3 – Base material strength analysis The dashboard is composed of various JMP platforms: Graph Builder, Distributions and ANOVA. The custom map shape[1] of the Graph Builder displays the two samples corresponding to each of the two plates and the position of the various cupping tests colored by strength. In the ANOVA, the overlap of the two diamond tips demonstrates that the plate can be considered as identical. The chart on the right shows that the strength variance is higher on operator side (OS). Once aggregated, data from the bottom distribution presents an average strength is 9.76±0.18 tons (at 2σ).